GUIDE
Plastics by FTIR: bands of PET, PE, PP, PS, PVC, PMMA and nylon
Infrared spectroscopy is widely used to characterize polymers because each family has a recognizable band pattern. The pattern, rather than one band, supports interpretation; bands also reveal crystallinity, conformation, oxidation and additives.
- The complete band pattern, rather than an isolated band, characterizes a polymer (PET, PE, PP, PS, PVC, PMMA, nylon…).
- Bands also reflect material condition: crystallinity, conformation, oxidation and plasticizers.
- ATR probes only the surface; additives, fillers, blends and microplastic matrices can hide or mimic bands.
1. Characteristic bands
Lesson 1: What is spectroscopy?Lesson 2: What is light?Molecular vibrations
| Polymer | Main bands (cm⁻¹) |
|---|---|
| PE (polyethylene) | 2915 and 2848 (C–H), 1470 and 1462, 730 and 720 (CH₂ rocking, a pair in crystalline chains) |
| PP (polypropylene) | 2950, 2917 and 2838; 1456 and 1376 (CH₃); 1167, 998, 973 and 841 |
| PS (polystyrene) | 3060 and 3026 (aromatic C–H), 1601, 1493 and 1452; 757 and 698 (monosubstituted ring) |
| PET (poly(ethylene terephthalate)) | 1715 (C=O), 1409, 1340, 1240, 1095, 1018, 872 e 723 |
| PVC (poly(vinyl chloride)) | 2970 and 2910, 1427, 1331, 1255, 1100, 960; C–Cl at 690 and 615 |
| PMMA (poly(methyl methacrylate)) | 1730 (C=O), 1435, 1240, 1190 e 1145, 985 e 750 |
| Polyamide (nylon 6 and 6,6) | 3300 (N–H), 2930 and 2860, 1640 (amide I), 1540 (amide II), 1260 |
| PC (polycarbonate) | 1770 (carbonate C=O), 1503, 1230, 1194 and 1164, 1015 and 830 |
| PU (polyurethane) | 3320 (N–H), 1730–1700 (urethane C=O), 1530, 1220 and 1100 |
| PTFE (Teflon) | 1210 e 1150 (C–F), 640 e 555 |
2. PE or PP?
Both have strong aliphatic C–H. PP has a CH₃ band at 1376 cm⁻¹ and a band pattern between 1170 and 840 cm⁻¹; PE has the 730 and 720 cm⁻¹ pair and almost no CH₃ at 1376. Ethylene–propylene copolymers show both features in varying proportions. Branching in low-density PE (LDPE) increases the CH₃ band at 1376 cm⁻¹, so this band alone cannot distinguish PP from LDPE: consider the full 1170–840 cm⁻¹ pattern.
3. Information beyond the polymer family
Besides indicating polymer family, bands reflect material condition: greater or lesser crystallinity, oxidation or plasticizer content. These indicators compare only samples measured using the same technique.
Explore further: crystallinity, conformation, oxidation and plasticizers
- Crystallinity. In PE, CH₂ rocking at ≈ 720 cm⁻¹ splits into a pair (730 and 720) in the orthorhombic crystalline phase through interactions between chains in the unit cell; the amorphous phase gives one band. In isotactic PP, bands such as 998 and 841 cm⁻¹ are associated with regular helical segments; their intensity tracks regularity (tacticity and crystallinity).
- PET conformation. Trans-conformation bands, such as 1340 and 973 cm⁻¹, and gauche bands (≈ 1370 and 896–898 cm⁻¹) help track crystallization: crystalline material is trans-rich, while amorphous material has a substantial gauche contribution.
- Oxidation and aging. In polyolefins, carbonyl formation creates a shoulder or band at ≈ 1715 cm⁻¹ (ketones, acids and esters). The carbonyl index (the ratio of carbonyl absorbance to a polymer reference-band absorbance, as defined by the author) is a relative indicator and compares only spectra obtained using the same technique and definition.
- Plasticizers. In flexible PVC, phthalates such as DEHP show aromatic-ester C=O at ≈ 1725 cm⁻¹ (≈ 1723 when dispersed in PVC), C–O bands at 1300–1000 cm⁻¹ and ortho-disubstituted ring bands (≈ 770–735 cm⁻¹), overlapping polymer bands.
4. ATR, depth and heterogeneity
In ATR, radiation penetrates about 0.5 to 3 µm (see ATR or KBr). The spectrum therefore represents the surface layer: an oxidized layer, coating, multilayer film or additives migrating to the surface can give a spectrum different from the material interior. To characterize the base polymer, compare the surface with a freshly cut interior. For heterogeneous samples, measure more than one location.
5. Interferences
- Additives and fillers: calcium carbonate (1430 and 875, 712), talc (OH at ≈ 3676 and broad bands at ≈ 1018), and silica (broad bands at 1100–1000 and ≈ 800) can obscure polymer bands.
- Mixtures and blends: bands combine and may be assigned to different components.
- Pigments and carbon black: absorb broadly, reduce the signal and distort the baseline (germanium helps in ATR).
- Microplastics in soil or sediment: the mineral matrix absorbs strongly between 1100 and 900 cm⁻¹, and plastic C–H bands may be below visual detection. Particles with biofilms show amide I and II bands (≈ 1650 and 1540) that do not belong to the plastic.
6. Practice
The platform includes an open industrial-polymer library (60 spectra of PET, HDPE, LDPE, PP, PS and PVC), useful as a ranking reference. Ranking is numerical comparison, not identification.
References
- Socrates, G. Infrared and Raman Characteristic Group Frequencies: Tables and Charts. 3rd ed. Chichester: Wiley, 2001.
- Stuart, B. H. Infrared Spectroscopy: Fundamentals and Applications. Chichester: Wiley, 2004.
- Smith, B. C. Infrared Spectral Interpretation: A Systematic Approach. Boca Raton: CRC Press, 1999.
- Käppler, A. et al. Analysis of environmental microplastics by vibrational microspectroscopy: FTIR, Raman or both? Analytical and Bioanalytical Chemistry, v. 408, p. 8377–8391, 2016. DOI 10.1007/s00216-016-9956-3.
Frequently asked questions
How can I distinguish PET from PMMA?
Both have C=O near 1720. PET shows 1715, 1240, 1095 and the aromatic pattern (1409, 872, 723); PMMA shows 1730 with 1190 and 1145 and no aromatic-ring bands.
How can I tell PE from PP?
PP has a CH₃ band at 1376 cm⁻¹ and bands between 1170 and 840 cm⁻¹. PE has the 730 and 720 cm⁻¹ pair. LDPE branching increases the 1376 band, so consider the whole pattern.
Does FTIR identify microplastics?
It can characterize the polymer family if the plastic is visible in the spectrum. In soil and sediment, the mineral matrix and biofilm can hide or mimic bands.
What is the carbonyl index?
It is the ratio of carbonyl-band absorbance (≈ 1715 cm⁻¹) to a polymer reference-band absorbance. It compares oxidation levels of samples measured using the same technique, provided the index definition is identical.
Ranges are typical tabulated values and vary with technique, physical state, matrix and instrument. This guide describes the polymer family and indicators of its condition; it does not identify substances with certainty.